Views: 0 Author: J-VALVES Publish Time: 2026-10-30 Origin: Site
"Stellite faced seats" is one of the most common hardfacing lines in a valve enquiry and one of the least complete. It does not say which Stellite, applied by which process, at what finished thickness, in how many layers, inspected how, or verified at what hardness. Two valves delivered against that same line can behave completely differently in a sandy stream: one still seals after three years, the other has a washed-out seat ring that no longer laps flat. This article sets out a selection method for hardfaced trim that starts from the erosion mechanism rather than the alloy name, with the numbers that make each decision defensible: impingement angle behaviour, the hardness ratio between particle and surface, the dilution and thickness rules of weld overlay, the 500 C boundary that separates cobalt alloys from tungsten carbide, and the specification clauses that decide whether the hardfacing survives machining, testing and commissioning.
Hardfacing and coating solve different problems with different physics, and enquiry documents that blur them get the wrong product at both ends. A hardfacing is a weld overlay or fused deposit, typically 1 to 4 mm thick when finished, metallurgically bonded to the substrate - the seat ring and the gate or disc are literally cast from a layer of the hard alloy. A coating is a micron-scale layer - a thermal spray deposit at 0.2 to 0.5 mm, an electroless nickel at 25 to 75 microns - mechanically or semi-metallurgically bonded. Micron-thick coatings answer corrosion, not abrasion; a film that can be scratched off with a file has no place carrying quartz sand at 20 metres per second.
The practical consequences follow from the bond and the thickness. A weld overlay can be machined, ground, lapped, and re-welded locally after damage; a sprayed carbide coating cannot be repaired in the field and must be stripped and re-applied. A weld overlay can be built 3 mm thick on a seat face that will see years of wear; a spray coating builds residual stress with thickness and is typically limited to a few tenths of a millimetre on trim. A weld overlay imposes weld heat - preheat, distortion, post-weld heat treatment questions on the finished body - while thermal spray runs near-cold and suits finished components. Neither is universally better, which is why the decision belongs in the specification, not in the quotation.
There is also a third family worth naming because enquiries increasingly ask for it: hard solid trim, such as a through-hardened 410 gate at 750 BHN or higher (the API trim 4 and 7 seats), or solid cemented carbide inserts on choke valves. Hard bulk material avoids every bonding question, but it cannot be machined after hardening, it is brittle in impact, and above roughly DN 100 an overlay is usually more economical than a solid hard part.
The first mistake in hardfacing selection is shopping by hardness number. Erosion is not abrasion between two flat surfaces; it is a stream of particles striking a surface at some angle, and the erosion rate depends on that angle in a way that inverts the ranking of materials.
For ductile materials - most steels, and relatively tough hardfacings - erosion peaks at a shallow impingement angle of roughly 20 to 30 degrees, where particles cut and plough across the surface. As the impact angle steepens toward 90 degrees, ductile erosion falls. For brittle materials - ceramics, hard carbide-rich microstructures, hard sprayed coatings - the opposite happens: material is removed by repeated impact fatigue, crack initiation and chipping, so erosion rises steadily with angle and is worst at normal incidence. A gate seat that sees particles sliding across the sealing face during every stroke lives in the shallow-angle regime, where cutting dominates and hardness wins. A seat in the flow stream behind a throttling point sees near-normal impacts at high velocity, where toughness matters as much as hardness. This is why a coating that beats Stellite 6 by a factor of three in a 30-degree dry grit test can lose to it in a 90-degree slurry test.
Velocity carries a heavier penalty than most buyers expect. Erosion follows a power law in particle velocity, and the exponent for metals is typically 2 to 2.5 (2.5 to 3 for ceramics). Double the velocity and the erosion rate rises four- to six-fold on metal trim. In a gate valve, velocity is concentrated in the small gap as the wedge approaches the seat: a valve that is stroked against a live differential at 15 metres per second gap velocity does not erode twice as fast as one stroked at 5 - it erodes nine or more times faster. Process operating points matter less than operating procedure; the single cheapest erosion countermeasure in a plant is to stop throttling with an isolation valve, or to accept that the downstream seat face of that valve is a consumable.
Particle size and concentration scale the problem. Erosion saturates at large particle sizes but has a threshold below which fine particles do little damage; a stream of 200 micron sharp sand at 2 percent by volume is a different duty from the same stream at 8 percent. Any hardfacing decision made without the particle data - size distribution, sharpness, hardness, concentration, velocity - is a guess with a hardness number attached.
The most useful single screening number in abrasive wear is the ratio of surface hardness to particle hardness. The commonly quoted transition band in tribology literature runs from about 0.8 to 1.3: when the surface is softer than 0.8 of the particle hardness, cutting and scratching proceed aggressively and the surface loses; above roughly 1.3, particles deform or round off against the surface and wear drops to a mild regime. Between the two lies a transition zone where ranking changes between materials and lab data should be trusted more than catalogue claims.
Put real numbers on it. Quartz sand, the dominant abrasive in produced water, river water and many slurries, sits near 1000 to 1200 HV. Stellite 6 is 380 to 490 HV as welded: a ratio of roughly 0.4 to 0.5, deep in the aggressive regime. The quartz cuts the cobalt alloy the way a file cuts brass - slowly in absolute terms, but relentlessly, and no heat treatment will change it. An HVOF tungsten carbide coating at 1100 to 1400 HV sits at a ratio of about 1.0 to 1.4: the transition zone, where the coating finally stands up to the mineral it faces. This is the arithmetic behind the industry pattern that a Stellite-faced seat gives acceptable life in clean steam and disappointing life in sandy water, and it cannot be argued away by specifying a "harder" Stellite.
Harder Stellite does exist and does help, within limits. Stellite 12 runs 45 to 51 HRC and Stellite 1 runs 50 to 58 HRC, with higher carbide volume for low-angle abrasion - but each step up trades away toughness, and the crack sensitivity of the weld overlay grows with it. Stellite 3 at 48 to 63 HRC is described by its own producer as nearly impossible to hardface crack-free. The hardness ratio says why the chase is futile: no cobalt alloy reaches the transition zone against quartz, so the additional carbides buy a longer ramp to the same failure mode. When the abrasive is softer than the surface - coal ash at 400 to 600 HV, hydrated lime, most polymer dusts - Stellite 6 is comfortably in the mild regime and is often the better total answer, because it brings toughness and galling resistance the carbides cannot.
Stellite is a trade name family of cobalt-chromium alloys, not one material, and the members differ exactly where selection matters. The matrix is cobalt, which is what gives the family its signature property set: hardness that survives temperature, low friction against mating metals, and resistance to galling, cavitation and many corrosive media.
Alloy | Key composition | Hardness as welded | Strongest against | Trade-off |
|---|---|---|---|---|
Stellite 6 | Co base, Cr 27-32 %, W 3-6 %, C 0.9-1.4 % | 36-45 HRC (380-490 HV) | Galling, sliding wear, cavitation, moderate erosion; all-round workhorse | Outmatched by quartz in abrasion; weld deposits are crack-sensitive on rigid parts |
Stellite 12 | Higher W and C than 6 | 45-51 HRC | Low-angle erosion, severe sliding, abrasion | Less impact tolerance; more crack-prone |
Stellite 1 | Highest C of the family | 50-58 HRC | Severe abrasion and low-angle erosion | Toughness drops noticeably; limited impact duty |
Stellite 3 | C about 2.3 % | 48-63 HRC | Extreme abrasion | Nearly impossible to deposit crack-free; almost no impact tolerance |
Stellite 21 | Co-Cr-Mo, low carbon (under 0.35 % C) | 27-40 HRC, work-hardens to about 48 | Cavitation, thermal and mechanical shock, metal-to-metal sliding | Not for hard particle abrasion; softer as deposited |
Two of these deserve emphasis because enquiries mix them up constantly. Stellite 6 is the industry-standard valve seat facing: it resists galling against stainless mating faces, retains useful hardness to about 500 C (with valve and steam service extending usefully to 540-650 C depending on load), resists cavitation, and can still be machined with carbide tooling and lapped to a sealing finish. It is the right answer for steam, hot oil, gas, and any metal-seated duty where the enemy is metal-to-metal wear and temperature, and the wrong answer for a sand-laden stream. Stellite 21 is the shock and cavitation specialist: low carbon, molybdenum-strengthened, work-hardening in service, and the usual facing where repeated impact or cavitation erosion destroys harder alloys - suction-side trim, letdown duty, high-pressure drops with flashing.
Cobalt itself carries two specification consequences. First, raw material cost is volatile and materially higher than nickel or iron alternatives, so a cobalt hardfacing should be justified by duty, not by habit - trim 1 or 4 is cheaper wherever the duty allows. Second, cobalt surfaces are routinely specified where the mating face must not gall: a 410 gate against a Stellite 6 seat slides with a low friction coefficient, which is exactly what a wedge needs during closure under load.
API 600 has encoded these decisions for decades in its trim chart, and quoting a trim number is a legitimate shorthand only if you know what it fixes and what it leaves open. The extract below shows the hardfaced rows most used in practice.
Trim number | Seat / disc facing | Base trim materials | Typical use | What the number does not fix |
|---|---|---|---|---|
Trim 1 | None - 410 throughout | 410 SS | Clean water, steam, general service | - |
Trim 4 | Hard 410 seats, 750 BHN minimum | 410 SS | High-pressure abrasive-clean service | Seat geometry, lapping finish |
Trim 5 | Hardfaced Stellite (seat and/or disc) | 410 SS | Steam, high temperature, erosion - the classic hard trim | Which Stellite, process, finished thickness |
Trim 5A | Hardfaced Ni-Cr | 410 SS | As trim 5, nickel-base hardfacing where required | Same as trim 5 |
Trim 8 | 410 with hardfaced seat | 410 SS | Refinery general service with one hardfaced face | Same as trim 5 |
Trim 12 | 316 with hardfaced Stellite | 316 SS | Chemical service plus temperature or wear | Same as trim 5 |
Trim 16 | 316 with hardfaced seat | 316 SS | Corrosive service needing a hard face | Same as trim 5 |
Note what the trim number does not control: alloy grade within "Stellite", application process, number of layers, finished thickness, dilution control, crack inspection, and final hardness. Two suppliers quoting "API trim 5" can deliver deposits differing by 300 HV, by half the thickness, and by whether anyone performed penetrant inspection after machining. The trim number is a family name, not a specification; the clauses in the last section of this article are what make it enforceable.
One pairing rule is worth fixing in every specification: dissimilar faces gall less than identical hard faces. The standard refinery arrangement is one hardfaced seat ring against a 410 disc (or one Stellite seat against one Stellite-faced wedge, where severe service justifies it), never two identical ultra-hard faces sliding dry. If both faces must be hardfaced, specify different compositions - for example Stellite 6 against a Ni-Cr hardfacing - so the friction couple has something to work with.
Against quartz and sharper minerals, the cobalt family runs out of hardness, and tungsten carbide enters. The dominant valve grade is WC-10Co-4Cr applied by HVOF (high-velocity oxy-fuel) spraying: 86 percent tungsten carbide by weight in a cobalt-chromium binder, deposited at particle velocities above 700 metres per second so the coating arrives dense and strongly bonded without melting the substrate.
Property | Stellite 6 weld overlay (PTA / GTAW) | HVOF WC-10Co-4Cr coating |
|---|---|---|
Hardness | 380-490 HV (36-45 HRC) | 1100-1400 HV0.3 |
Bond to substrate | Metallurgical fusion, substrate-limited | Mechanical/semi-metallurgical, 70-83 MPa typical (ASTM C633) |
As-deposited porosity | Near zero (fully fused) | Under 1 percent on a well-run HVOF process |
Finished thickness on trim | 1-4 mm; many specs require at least 1.6 mm finished | Typically 0.2-0.5 mm finished; residual stress limits build-up |
Max continuous service temperature | About 500 C hardness retention; valve/steam use to 540-650 C | About 450-540 C; WC oxidises and decarburises above roughly 500 C |
Corrosion of the surface layer | Good in many acids and wet H2S | Good with the 4 % Cr binder (1000 h plus salt spray); WC-12Co without Cr is not |
Finishing | Machinable with carbide tooling, then lapped | Diamond grinding only; grind and superfinish to Ra 0.05-0.2 microns |
Field repair | Re-weldable locally after preparation | Not field repairable; strip and re-spray |
Geometry limits | Needs access for the torch; heavy preheat on large bodies | Line-of-sight process: no internal bores under about 50 mm, spray angles below 30 degrees not feasible |
Impact tolerance | Good - tough cobalt matrix | Limited - chipping and spalling under repeated impact |
The table exposes the three ways HVOF carbide fails in valve service, and all three are process or specification failures, not material failures. First, thickness at edges: residual stress grows with thickness, and stress concentrates where the seat face meets a corner or a step. A coating pushed to 0.8 mm to "buy margin" frequently cracks or lifts exactly there; the honest practice is a thickness the applicator has qualified, with edge geometry (chamfers, radii, blending) agreed before spraying. Second, temperature: WC starts oxidising and decarburising above roughly 500 C, and the coating loses both hardness and binder integrity - steam service belongs to cobalt alloys, not carbides. Third, impact: under repeated normal impacts the WC grains are crushed and displaced and the coating spalls in flakes; a slug of weld spatter through a ball valve does more damage to a sprayed seat than a year of sand.
Two chemistry notes complete the picture. The 4 percent chromium in WC-10Co-4Cr is not cosmetic: it is what lets the coating survive salt water and sour condensate, where the older WC-12Co corrodes its own binder and drops carbide grains. And spray process control matters more than powder datasheets: in poorly controlled processes a large fraction of the WC can decompose to brittle W2C during spraying, which quietly degrades abrasion performance; HVOF's lower process temperature is precisely why it dominates this application. Buy the applicator's process qualification, not just the powder name.
Where the duty is erosion at high temperature - fly ash, fluidised-bed and FCC slide valve duties - the carbide of choice shifts to chromium carbide in a nickel-chromium binder (Cr3C2-NiCr), which gives up some room-temperature hardness but serves usefully to about 870 C, well past the point where tungsten carbide has begun to destroy itself. This is the third hardfacing family, and it should be named in enquiries about hot gas erosion rather than left to the supplier's judgement.
A weld overlay is a casting process on a finished part, and its quality is decided at the melt pool. The substrate always mixes into the first layer - that is what fusion means - and the mixed first layer is softer and less corrosion-resistant than the filler: a carbon steel substrate dilutes the deposit's carbon and chromium, and a stainless substrate brings iron and nickel. Typical dilution figures run in the tens of percent for common arc processes and in the single digits for plasma transferred arc (PTA) and laser cladding, which is why PTA has become the preferred process for seat rings where hardness must be guaranteed after machining.
Practice follows directly: hardfaced seats carry at least two layers, and the finished surface is machined out of the second (or later) layer, so the hardness guarantee belongs to the deposit after machining, not to the as-deposited wire. The specification should state the minimum finished thickness at the sealing face (1.6 mm is a widely used floor for weld overlay seats), the number of layers, and - critically - the hardness to be measured on the finished face, with microhardness (HV or converted HRC) rather than a rebound tester that reads a mix of layers.
Cracking is the second gate. Cobalt hardfacings are crack-sensitive: welds on rigid seat rings or large wedges cool under constraint and can crack radially or in a checkered pattern, and some alloys (Stellite 3, and any deposit approaching 60 HRC) are practically unbuildable crack-free. Preheat and slow cooling reduce the risk; they do not remove it. That is why the acceptance test is penetrant inspection after final machining and lapping - the point where sub-surface cracks have been opened to the surface - and not before. A supplier who offers a PT report "as welded" but not "as machined" has skipped the only inspection that tells you anything.
Heat input also reaches the parent body. A weld overlay on a finished CF8M body is a post-weld heat treatment decision on the assembly: sensitisation, distortion of lapped faces, and stress relief of the seat pocket all enter the conversation, which is one more reason spray processes (near-cold) exist for finished components. If an overlay must go onto a finished body, agree the thermal plan before purchase order, not after the first warped bonnet.
Temperature quietly reorders the ranking. Stellite 6 keeps useful hardness to about 500 C and stays in service as valve trim to 540-650 C depending on load, because the cobalt matrix and its carbides do not lose their structure. Tungsten carbide coatings, harder at room temperature, begin to oxidise and decarburise above roughly 500 C - the binder degrades, the coating loses integrity, and hardness readings become meaningless. Chromium carbide takes over from there to about 870 C.
So the temperature map is simple to write into a specification: below 450 C and abrasive - HVOF WC-10Co-4Cr. Around 500 C with metal-to-metal wear, steam, cavitation - Stellite 6 or 21. Above 540 C with erosive gas - Cr3C2-NiCr. Above 870 C there is no spray coating worth buying, and the answer is refractory metal trim or a redesign of the duty. An enquiry that says "hardfaced trim for 550 C steam" has answered its own alloy question: any WC line item in the quotation for that duty should be challenged.
The families above reduce to a short decision table when you classify by dominant mechanism, temperature and medium.
Service | Dominant mechanism | Trim answer | Notes |
|---|---|---|---|
Sandy wellhead crude, choke and gate duties (API 6A) | Low-angle abrasion, quartz | HVOF WC-10Co-4Cr on gate faces and seats, or welded WC composite on chokes | Only the carbide reaches the hardness transition; Stellite ramps slowly to the same failure |
Wet CO2 with sand, 410 body trim | Abrasion plus corrosion | WC-10Co-4Cr (the Cr binder matters) on 410 or 316 trim | Avoid WC-12Co in any wet chloride or sour condensate |
Superheated steam, boiler feed, letdown | Metal-to-metal wear, cavitation, temperature | Stellite 6 seats; Stellite 21 where impact or flashing dominates | Trim 5 territory; carbide is disqualified above 500 C |
Fly ash, FCC and fluidised-bed slide valves, 550-850 C | Hot erosion at temperature | Cr3C2-NiCr overlay or coating | The only spray family alive past the WC limit |
Slurry, low velocity, large soft particles | Abrasion with impact | Rubber or polyurethane lined body plus carbide-faced metal trim at the sealing faces | Elastomers absorb impact that hard coatings cannot; see rubber and PTFE linings for the lining side |
Corrosive service with wear (acids, chlorides plus velocity) | Corrosion-dominated | Alloy body or 316 trim with Stellite facing (trim 12/16), or Ni-base hardfacing | Hardness cannot substitute for corrosion resistance; the facing only buys wear life |
Sour service (wet H2S) | Wear plus sulphide constraints | Ni-Cr hardfacing (trim 5A/8A) or Stellite; hardness above 22 HRC handled per ISO 15156 qualification | The 22 HRC cap applies to carbon and low-alloy steels; hardfaced faces follow their own qualification route - state it in the datasheet |
Two cross-checks keep the table honest. First, the leakage class you accept is tested on the finished hardfaced seat, so the facing, the machining and the test are one system, not three purchases. Second, procedure: an isolation valve throttled regularly will erode any trim, and the correct fix is procedural or a control valve, not a harder seat.
When hardfaced trim comes back, the damage pattern identifies the mechanism - and therefore the fix - more reliably than any incident report.
Signature on the seat face | Mechanism | Typical root cause | Effective response |
|---|---|---|---|
Parallel score lines across the face, aligned with flow; band deepest where the wedge sat in throttling | Cutting erosion at shallow angle | Throttling an isolation valve; sand in a clean-service line | Stop throttling or expect consumable seats; upgrade to carbide if Stellite shows this |
Polished ring with ragged pitted edges, sponge-like metal | Cavitation | Pressure drop across the seat during stroking | Stellite 21 or redesign the pressure stage; harder alloy will chip faster |
Flakes of coating lifted, substrate polished or corroded beneath | Spalling of a sprayed layer | Thickness or edge stress, poor surface prep, grinding heat, impact | Re-qualify applicator process; reduce thickness; blend edges; diamond grinding with coolant |
Radial or checkered cracks in the overlay | Weld cracking | Constraint, missing preheat, alloy too hard for the geometry | PT after machining in the spec; step down to Stellite 6; PTA or laser process |
Smears and transferred material, sticking, rising torque over strokes | Galling | Identical hard faces sliding dry; overspeed closure | Dissimilar pairing (one face hardfaced, or different hardfacings); check actuator speed |
Uniform thinning of the finished face with no cracks or scoring | Corrosion plus sliding wear (tribocorrosion) | Facing chosen for wear, medium attacking the binder or matrix | Re-select for corrosion: WC-12Co gives way to WC-10Co-4Cr or a Ni binder; Stellite to higher alloy |
The spalling signature deserves one more line, because it is the most litigated: a sprayed coating that lifts is almost never evidence that "spray does not work" - it is evidence that the coating exceeded a qualified thickness, or was ground dry and overheated, or was applied over contamination. Asking for the applicator's process qualification (spray parameters, grit profile, bond test coupon result) at purchase order stage costs one email and removes the argument later.
Everything above compresses into a handful of clauses that a procurement engineer can paste into a datasheet. Each targets a specific failure of communication observed repeatedly in this product family.
Name the alloy and the family: "Stellite 6 (UNS R30006)" or "HVOF WC-10Co-4Cr (86/10/4)" - never "hardfaced" alone.
Name the process: PTA or GTAW weld overlay, or HVOF spray; the process sets dilution, thickness and heat-input limits.
State minimum finished thickness at the sealing face (for example 1.6 mm for weld overlay seats, 0.3 mm for sprayed coatings) and the number of overlay layers.
Require hardness measured on the finished, machined face by microhardness, with a limit and a certificate - not as-deposited values from the powder datasheet.
Require penetrant inspection of all hardfaced faces after final machining and lapping, with the report referenced to serial numbers.
For overlays on finished bodies, require the thermal plan (preheat, interpass, PWHT if any) submitted for approval before application.
For HVOF coatings, require the applicator's process qualification: grit blast profile, spray parameters, and bond strength from a coupon of the same batch (70 MPa or better typical).
Fix the mating pair: which face is hardfaced, which is not, and the compositions on each side (dissimilar pairing to control galling).
State the design temperature at the seat; any tungsten carbide line item above 500 C should be rejected at bid stage.
State the leakage class and test medium for the assembled valve, so the hardfacing, lapping and testing form one acceptance chain; see the API 598 seat test sequence for how the finished seat is actually proven.
For sour service, reference ISO 15156 qualification for the hardfaced faces and name the trim (5A/8A) rather than leaving hardness compliance implicit.
Repair policy: state whether Stellite faces may be locally re-welded after damage and re-inspected, and confirm sprayed coatings are not field repairable - spares policy follows from this line.
A buyer who writes these twelve lines has specified more hardfacing engineering than most enquiries that run to forty pages, because every line closes a gap that quotation documents otherwise fill with the supplier's cheapest process. The gate valve range on this site can be configured with Stellite or carbide-faced seats against these clauses, and the technical article library collects the companion pieces on seal design, testing and materials.
Should both seat faces be hardfaced, or only one?
Dissimilar faces gall less than identical hard faces, so the default refinery arrangement is one hardfaced seat ring against an unfaced 410 or 316 disc - which is exactly what trim 8 and trim 12 encode. When the duty is severe enough to face both sides (trim 5, 13 territory), specify different compositions on the two faces, for example Stellite 6 against a nickel-chromium hardfacing, so the friction couple keeps a lubricating difference. Two identical ultra-hard faces sliding dry against each other is the classic recipe for galling smears and a torque curve that climbs stroke by stroke.
Is a 55 HRC hardfacing always better than a 40 HRC one?
No, and in some duties it is worse. Erosion at shallow angles rewards hardness, but erosion at normal incidence removes brittle material by impact fatigue and cracking, so a harder deposit can lose to a tougher one behind a throttling point or under cavitation. Every step up the hardness ladder also raises crack sensitivity in the weld overlay - the hardest cobalt grades are described by their own producer as nearly impossible to deposit crack-free. Choose by mechanism first: Stellite 6 for sliding wear, cavitation and temperature; tungsten carbide when quartz hardness demands it; never hardness as a standalone criterion.
Why did an HVOF tungsten carbide coating spall off the seat after a few months?
Almost always a process or specification failure, not a material failure. The usual causes are a thickness beyond what the applicator qualified (residual stress grows with thickness and peaks at edges and steps), grinding without coolant that overheated the layer, surface preparation or contamination failures, and impact the coating was never meant to take. Ask for the applicator's process qualification - blast profile, spray parameters, and a bond-strength coupon from the same batch, typically above 70 MPa - and agree edge geometry before spraying. A lifting coating usually points to one of those, and the fix is procedural rather than a different alloy.
Can hardfaced seats be repaired in the field?
It depends entirely on the family. A Stellite weld overlay can be locally re-welded after grinding out the damage, then re-machined, re-lapped and re-inspected by penetrant testing - that repair route is one of its main advantages. A sprayed carbide coating cannot be repaired in the field at all: the coating must be stripped back to sound substrate and re-sprayed by a qualified shop, which usually means sending the trim out. Write the repair policy into the specification, because it decides your spare-trim strategy for the whole plant.
What should a hardfacing purchase specification actually contain?
Twelve lines carry most of the value: named alloy with UNS or composition (Stellite 6 / UNS R30006, or WC-10Co-4Cr 86/10/4); named process (PTA or GTAW overlay, or HVOF); minimum finished thickness at the sealing face and layer count; hardness measured on the finished machined face by microhardness with a certificate; penetrant inspection after final machining and lapping; the thermal plan for overlays on finished bodies; process qualification for sprayed coatings including bond coupon; the mating pair of faces and their compositions; seat design temperature so any tungsten carbide above 500 C is rejected at bid; leakage class and test medium tying facing, lapping and testing into one acceptance chain; ISO 15156 reference for sour service; and the repair policy. A trim number alone fixes none of these.